Projects per year
Abstract
Ammonia is a promising fuel due to its high volumetric energy density and carbon-free nature. It is already produced on a large scale through the Haber–Bosch process and has a well-established transportation network, making it an attractive candidate as an energy vector in future sustainable energy systems. Solid oxide cells (SOCs) have been investigated for direct ammonia conversion due to their high efficiency. While SOCs have demonstrated stable operation on ammonia for thousands of hours, most previous studies have focused on single-cell testing and have not fully addressed the influence of ammonia on the auxiliary components used in practical stack configurations.
The impact of ammonia on auxiliary stack components, particularly with respect to corrosion and nitridation, remains poorly understood and may represent a key limitation for the practical implementation of SOC systems operated on ammonia. One of the main objectives of this thesis is to investigate ammonia-induced degradation of SOC stack components under stack-relevant conditions and its impact on the lifetime of stainless steel auxiliary components.
In this thesis, the compatibility between ammonia and SOC stack components is investigated, with particular focus on ammonia corrosion of stainless steels commonly used for interconnectors or balanceofplant components. Ferritic stainless steels (Crofer 22 APU, Crofer 22 H, and AISI 441), together with additional steels and Ni-based alloys were evaluated. A combination of single-atmosphere exposure testing, dual-atmosphere testing, and single repeating unit (SRU) experiments were employed to evaluate material degradation under stack-relevant conditions. Tests were carried out at typical SOC temperatures between 600 and 850 °C, and the gas composition was representative of an ammonia recirculation feed.
The results show that ammonia corrosion of stainless steels strongly depends on temperature and gas composition. At temperatures lower than 700 °C, chromium nitride formation caused significant structural degradation of the steel. At 750 °C and above, ferritic stainless steels exhibited minimal nitridation in exposure tests, although nitridation was still observed in SRU testing. In contrast, operation at 800 °C suppressed chromium nitride formation in the investigated systems. Mass gain was not a reliable indicator of nitridation formation in stainless steel, since severe local nitridation was detected for steels experiencing a mass gain below 0.5 mg/cm2. Several coatings were evaluated to mitigate the nitride formation, with Al-, Ce-, Gd-, and Y-based coatings showing the most promising behavior in the exposure tests. Ni-rich alloys containing more than 60 w% Ni also demonstrated improved resistance to ammonia corrosion compared to conventional stainless steels, such as Crofer 22 APU and AISI 441.
SRU testing confirmed that nitridation can occur in stack environments and may lead to significant expansion of stainless steel interconnectors, increasing the risk of mechanical failure. However, the electrochemical performance of the SOC itself was only moderately affected by ammonia operation compared to operation in precracked ammonia (3:1 H2/N2). Only a moderate increase in degradation rate was observed compared to single-cell testing under precracked ammonia conditions (11.4 vs 18.4 mV/kh at 750 °C and 0.5 A/cm2), indicating that the SOC maintains stable electrochemical performance. The results indicate that auxiliary components, particularly stainless steel interconnectors and Nibased contact materials, are the primary limiting factors for long-term SOC operation on ammonia. The formation of chromium nitride in the stainless steel interconnectors deprives them of the ability to form a protective Croxide scale and thus limits the lifetime of the stainless steel. This also causes uneven expansion of the interconnector, increasing the thickness of the plate at the inlet by 13% compared to the outlet. The Ni contact elements also showed a porous nature near the inlet, indicating expansion as a consequence of exposure to ammonia.
Overall, this work demonstrates that SOC systems can operate on ammonia, but careful control of operating temperature, gas composition, and materials selection is required to mitigate nitridation and ensure long-term stack durability.
The impact of ammonia on auxiliary stack components, particularly with respect to corrosion and nitridation, remains poorly understood and may represent a key limitation for the practical implementation of SOC systems operated on ammonia. One of the main objectives of this thesis is to investigate ammonia-induced degradation of SOC stack components under stack-relevant conditions and its impact on the lifetime of stainless steel auxiliary components.
In this thesis, the compatibility between ammonia and SOC stack components is investigated, with particular focus on ammonia corrosion of stainless steels commonly used for interconnectors or balanceofplant components. Ferritic stainless steels (Crofer 22 APU, Crofer 22 H, and AISI 441), together with additional steels and Ni-based alloys were evaluated. A combination of single-atmosphere exposure testing, dual-atmosphere testing, and single repeating unit (SRU) experiments were employed to evaluate material degradation under stack-relevant conditions. Tests were carried out at typical SOC temperatures between 600 and 850 °C, and the gas composition was representative of an ammonia recirculation feed.
The results show that ammonia corrosion of stainless steels strongly depends on temperature and gas composition. At temperatures lower than 700 °C, chromium nitride formation caused significant structural degradation of the steel. At 750 °C and above, ferritic stainless steels exhibited minimal nitridation in exposure tests, although nitridation was still observed in SRU testing. In contrast, operation at 800 °C suppressed chromium nitride formation in the investigated systems. Mass gain was not a reliable indicator of nitridation formation in stainless steel, since severe local nitridation was detected for steels experiencing a mass gain below 0.5 mg/cm2. Several coatings were evaluated to mitigate the nitride formation, with Al-, Ce-, Gd-, and Y-based coatings showing the most promising behavior in the exposure tests. Ni-rich alloys containing more than 60 w% Ni also demonstrated improved resistance to ammonia corrosion compared to conventional stainless steels, such as Crofer 22 APU and AISI 441.
SRU testing confirmed that nitridation can occur in stack environments and may lead to significant expansion of stainless steel interconnectors, increasing the risk of mechanical failure. However, the electrochemical performance of the SOC itself was only moderately affected by ammonia operation compared to operation in precracked ammonia (3:1 H2/N2). Only a moderate increase in degradation rate was observed compared to single-cell testing under precracked ammonia conditions (11.4 vs 18.4 mV/kh at 750 °C and 0.5 A/cm2), indicating that the SOC maintains stable electrochemical performance. The results indicate that auxiliary components, particularly stainless steel interconnectors and Nibased contact materials, are the primary limiting factors for long-term SOC operation on ammonia. The formation of chromium nitride in the stainless steel interconnectors deprives them of the ability to form a protective Croxide scale and thus limits the lifetime of the stainless steel. This also causes uneven expansion of the interconnector, increasing the thickness of the plate at the inlet by 13% compared to the outlet. The Ni contact elements also showed a porous nature near the inlet, indicating expansion as a consequence of exposure to ammonia.
Overall, this work demonstrates that SOC systems can operate on ammonia, but careful control of operating temperature, gas composition, and materials selection is required to mitigate nitridation and ensure long-term stack durability.
| Original language | English |
|---|
| Place of Publication | Kgs. Lyngby |
|---|---|
| Publisher | Technical University of Denmark |
| Number of pages | 304 |
| Publication status | Published - 2025 |
Fingerprint
Dive into the research topics of 'SOFC and Interconnector Stability in NH3'. Together they form a unique fingerprint.Projects
- 1 Finished
-
SOFC and interconnector stability in NH3
Jacobsen, A. B. (PhD Student), Sun, X. (Main Supervisor), Hendriksen, P. V. (Supervisor), Njodzefon, J.-C. (Examiner) & Talic, B. (Examiner)
15/11/2022 → 14/11/2025
Project: PhD
Cite this
- APA
- Author
- BIBTEX
- Harvard
- Standard
- RIS
- Vancouver